Dear All,

We have an air patenting furnace 13 meters long with 3 burners to control the temperature and air fans from 2 sides, but sometimes patenting wire is cracked.

What is the suitable air pressure to get fine pearlite?

Thank you for your kind attentions,
The administrator has disabled public write access.

Re: Air Patenting 2 years 11 months ago #871

To obtain fine perlite ( on high carbon wires), the wire should heat uniformily up to fully transformation temperature where it is fully austenized (+,-) 800 oC then sudenlly in few seconds the material should decrease temperature ( +,-)500oc. . The conditions for different carbon contents can be obtain in the TTT curves ( Temperatur, Time ,Transformatio). WAI has several presentations on the subject can be seen on his web page

Eduardo Anaya
Senior Consultant
INDEPA S.C.
Mexico City
Tel(011-52)555-407-7451
This email address is being protected from spambots. You need JavaScript enabled to view it.
The administrator has disabled public write access.
Time to create page: 0.162 seconds