make up natural cara make up make up tutorial make up korea make up minimalis make up artis make up mata belajar make up make up wardah alat make up makeup forever indonesia makeup artist jakarta tips make up barbie make up natural make up make up wajah make up pesta make up syahrini makeup mata makeup minimalis peralatan make up make up cantik make up mac make up kit jual make up make up sederhana perlengkapan make up gambar make up vidio make up cara makeup minimalis wardah make up make up pac make up glamour cara memakai makeup make up panggung harga make up make up modern make up alami make up dasar pixy make up make up muslimah make up oriflame make up jepang makeover cosmetic make up ultima make up sariayu grosir make up makeup fantasi makeup pesta tas makeup langkah make up make up pria make up malam alat makeup tahapan make up produk make up shading make up mak up make up kebaya make up jilbab make up inez make up simpel contoh make up cara ber makeup makeup wajah tanpa make up make up terbaru toko make up mac makeup indonesia make up soft urutan make up trik make up makeover makeup brand gusnaldi make up paket make up panduan make up jual makeup brush make up bagus alat2 make up make up gusnaldi aplikasi make up alat alat makeup dasar make up inez make up peralatan makeup make up wanita make up berjilbab make up tebal sejarah make up make up maybeline make up branded make up siang tata cara makeup reseller make up make up muslim make up maybelin warna make up tips make up artist rias make up make up mata make up artis belajar make up make up artist kursus make up kuas make up make up forever indonesia jual make up mac indonesia make up make up artist indonesia harga make up forever jual make up online make up pac make up forever jakarta make up oriflame jual make up forever make up online shop indonesia harga make up sekolah make up grosir make up harga make up maybelline jual make up murah make up terbaru mak up mac make up indonesia sofia make up make up kit murah mac makeup indonesia produk make up jual make up kit make up store indonesia make up forever academy jakarta toko make up online jual make up set jual make up mac make up beauty jual make up branded produk make up mac make up forever harga make up mac indonesia produk make up artis jual make up palette produk make up forever make up palette murah before after make up pengantin before after make up sendiri before n after hasil makeup contoh make up karakter contoh riasan pengantin before n after harga make up wisuda harga make up artist harga make up forever make up wisuda rias wisuda di jogja Daftar harga make up forever daftar harga make up mac daftar harga kosmetik make up forever makeup wisuda harga makeup wisuda kursus make up di yogyakarta kursus make up di jogja kursus make up jogja kursus make up yogyakarta kursus kecantikan di yogyakarta kursus kecantikan di jogja kursus make up artist di jogja kursus rias pengantin di jogja kursus rias di yogyakarta kursus tata rias di yogyakarta rias pengantin muslim jogja jasa kreasi jilbab wisuda yogyakarta jasa rias make up wisuda murah bagus bisa dpanggil tempat make uf di jigja yang bagus rias wisuda murah dan berkualitas yogyakarta pakar kreasi jilbab di jogja make uper natural yogya make up wisuda hijab area jogja make up dan kreasi jilbab yang bagus di jogja jasa make up natural untuk wisuda jogja makeup jogja make up jogja makeup yogyakarta make up yogyakarta makeup wisuda jogja make up wisuda jogja make up wisuda yogyakarta makeup wisuda yogyakarta
Search - Content
Search - People/Events
Search - Forums
Search - Newsfeeds



jobcenterbanner

FacebookLinkedinPinterestYoutube
Welcome, Guest
Username: Password: Remember me
Nonferrous topics such as copper and aluminum, annealing, etc. go here.
  • Page:
  • 1
  • 2

TOPIC: 10%PTIR

10%PTIR 2 years 6 months ago #1499

No place for precious metals so I am trying here. Does anyone have any tricks or tips on pointing fine (<.002 inch ) 10%PTIR for wire drawing purposes. I have tried aqua regia , NAOH , and mechanical methods. None seemed to be very efficient or safe. Any comments or ideas are much appreciated.
Tech 1
The administrator has disabled public write access.

Re: 10%PTIR 2 years 6 months ago #1500

Hi there Tech1,

Long time!
On the assumption that the acronym 10% PTIR stands for an alloy of 90% platinum and 10% iridium, I have moved this over to the Nonferrous Section and made sure it was at the front of the line.

Hopefully somebody will give you an answer to your rather exotic question.

Best regards,
Peter J. Stewart-Hay
Principal
Stewart-Hay Associates
www.Stewart-Hay.com
The administrator has disabled public write access.

Re: 10%PTIR 2 years 6 months ago #1501

Here is some information I learned from the H. Cross Company:

"90/10 Platinum/Iridium Physical Properties (Annealed Condition)

Density 21.53 g/cc
Mechanical Properties
Ultimate Tensile Strength 55,100 PSI
Electrical Resistivity 0.000025 ohm-cm
Hardness Brinell 130

The alloy 90/10 platinum iridium, containing 10 per cent iridium, has very good all round manufacturing characteristics: it can be cast, welded, machined and stamped; it is ductile and malleable; can be hardened through working; and does not readily oxidize. Because of these advantages 90/10 Plat Iridium has traditionally been one of the most important jewelry alloys used in the USA, although there has recently been a swing toward alloys of 95/5 Platinum Iridium. Some manufacturers in Germany and Japan also prefer the 95/5 alloy. The 80/20 Plat Iridium alloy is very hard and dense, and is sometimes used in the production of fine wire work."

The melting point of 90/10 platinum iridium alloy is 1800C or 3272F. For comparison, the melting point of copper is 1083C or 1981.4F.

Is the wire already work hardened when you want to point it or is it a lot less ductile than is suggested here?

Best regards,
Peter J. Stewart-Hay
Principal
Stewart-Hay Associates
www.Stewart-Hay.com
The administrator has disabled public write access.

Re: 10%PTIR 2 years 6 months ago #1502

hi ya vettecoupe,
Yup, long time no talk. Still doing the same ole stuff.
Anyway, It really doesn't matter if the PTIR is hard or soft. The size of it ( <.002 ) is the problem for working with. Traditionally, we would use somesort of eletrochemical pointing method with other alloys but the PTIR will not work that way. I have also seen methods of scrapping the wire to make a point but the size of this wire is preventing that as well. There are so many ways of pointing larger wires but the small stuff is always very difficult or there is some silly trick that someone came up with that is usually very efficent and easy. Now, thats what Iam looking for. So, If anyone has some tricks up their sleeve, please pass them on.
The administrator has disabled public write access.

Re: 10%PTIR 2 years 6 months ago #1503

Hello Tech1.

Have you tried heating the wire. Since it is fine, take about 12 -18 inches. grip it so that it will not slip out of you fingers, hold the middle of the 12-18 inc piece over a butane torch---same one you might use for brazing wire. When you see the wire start to get red move your hands further apart until the wire breaks. It should have a nice taper to it that ou would be able to stick into the die. Don't heat it too much or you might not be able to grab it and pull it through the die.
The administrator has disabled public write access.

Re: 10%PTIR 2 years 6 months ago #1504

Tried the heating method. Not so good. Wire becomes brittle and does not point. Another thing is 12-18 inches of wire becomes very expensive.